Hot Work Tool Steels

1.2365 Standards DIN X32CrMoV3-3

Chemical Composition

% C0,33
% Si0,35
% Mn0,35
% Cr2,90
% Mo2,75

Applications

Used as a piston in the injection of copper and alloys

Heat Treatment Properties

  • Stress Relief °C
    650
  • Soft Annealing °C
    780-810
  • Delivery Hardness
    +A / max. 229

Hardness

  • Austenitizing °C 
    1010-1050 
  • Cooling
    Oil, Fluid bed , Air

Hardness After Hardening

  • HRC
    51
Tempering °C 100 200 300 400 500 550 600 650 700
HRC 51 50 49 49 49 50 48 41 29
Tensile Strenght N/mm2 1730 1680 1620 1620 1620 1680 1570 1300 940